低温玻璃浆料圆片级真空封装的研究
摘要
研究了玻璃浆料在低温下真空封装MEMS器件的工艺。封装过程中
采用了丝网印刷技术
丝网的线宽设计为100μm
印刷后玻璃浆料线宽为160μm左右
从而能够减小封装器件的尺寸
节省成本;另外
对玻璃浆料键合工艺做了研究
找到了较好的工艺条件
采用该工艺(预烧结温度425℃
键合温度430℃)
得到的封装结构具有较高的封接强度(剪切力>20 kgf)和良好的真空度
测得的漏率为10-9 cm3/s。
Abstract
Glass frit packaging is important for MEMS devices vacuum packaging.Screen printing is applied in package